Flux Packaging

Diameters / Packaging

Diameters
22.7 KG BAG
Flux ED032990

Lincolnweld® WTX

Submerged Arc Welding (SAW) | ED032990

Special Neutral Flux

DETAILS

  • Neutral submerged arc welding flux designed to meet the specific requirements of wind tower welding applications
  • Recommended for use with Lincolnweld® L-61 electrode on both longitudinal and circumferential seam welds
  • Capable of producing weld deposits with impact properties exceeding 27 J (20 ft·lbf) @ -62°C (-80°F)
  • Smooth bead profile to achieve excellent toe angles, tie-in, and bead appearance on interior and exterior applications

Features

  • Neutral submerged arc welding flux designed to meet the specific requirements of wind tower welding applications
  • Recommended for use with Lincolnweld L-61 electrode on both longitudinal and circumferential seam welds
  • Capable of producing weld deposits with impact properties exceeding 27 | (20 ft lbf) at --62 C (-80 F)
  • Smooth bead profile to achieve excellent toe angles, tie-in, and bead appearance on interior and exterior applications
  • Actual (Type 3.1) certificates for each lot of flux showing chemical composition, particle size and moisture level are available in the certificate center of lincolnwelectric.com

Service Information

Documentation

You May Also Need

BEFORE USE, READ AND UNDERSTAND THE SAFETY DATA SHEET (SDS) FOR THIS PRODUCT AND SPECIFIC INFORMATION PRINTED ON THE PRODUCT CONTAINER. SDS Search page

MECHANICAL PROPERTIES

Wire Classification Postweld Heat Treatment Yield Strength @ 0.2% Offset
MPa (ksi)
Tensile Strength
MPa (ksi)
Elongation
%
Charpy V-Notch
J (ft-lbs) @ -40°C (-40°F)
Charpy V-Notch
J (ft-lbs) @ -50°C (-60°F)
Charpy V-Notch
J (ft-lbs) @ -62°C (-80°F)
Lincolnweld® L-50® F7A6-EM13K As-welded 500 (73) 590 (86) 29 89 (66)
Lincolnweld® L-56® F9A6-EH11K-G As-welded 600 (87) 700 (101) 26 66 (49)
Lincolnweld® L-61® F6P8-EM12K-H8 1 hour @ 620°C (1150°F) 360 (52) 460 (67) 36 213 (157)
Lincolnweld® L-61® F7A8-EM12K-H8 As-welded 410 (60) 520 (75) 31 88 (65)
Lincolnweld® L-70 F8A4-EA1-A3-H8 As-welded 530 (77) 610 (88) 26 64 (47)
Lincolnweld® LA-71 F7A6-EM14K-H8 As-welded 550 (80) 630 (91) 27 138 (102)
Lincolnweld® LA-75 F7A4-ENi1K-G-H8 As-welded 500 (72) 590 (86) 29 144 (106)

DEPOSIT COMPOSITION

Wire Classification %C %Cr %Cu %Mn %Mo %Ni %P %S %Si %Ti Diffusible Hydrogen
mL/100g Weld Metal
Lincolnweld® L-50® F7A6-EM13K 0.05 0.08 2.12 0.015 0.004 0.45
Lincolnweld® L-56® F9A6-EH11K-G 0.05 0.05 0.08 2.47 0.01 0.03 0.014 0.003 0.76
Lincolnweld® L-61® F6P8-EM12K-H8 0.06 0.11 1.57 0.014 0.008 0.25 5
Lincolnweld® L-61® F7A8-EM12K-H8 0.06 0.07 1.72 0.012 0.008 0.32 4
Lincolnweld® L-70 F8A4-EA1-A3-H8 0.05 0.08 1.55 0.52 0.011 0.009 0.23 5
Lincolnweld® LA-71 F7A6-EM14K-H8 0.06 0.08 2.00 0.012 0.005 0.62 0.02 5
Lincolnweld® LA-75 F7A4-ENi1K-G-H8 0.06 0.03 0.10 1.93 0.00 0.86 0.012 0.006 0.46 5

FLUX COMPOSITION

Classification %Al2O3 %CaF2 %CaO %FeO %K2O %MgO %MnO %Na2O %SiO2 %TiO2 %ZrO2
Typical Result 24 13 4 3 1 23 8 2 18 2 2